- 17
- Sep
Brick mejupụtara obere ihe na -akpụ akpụ maka ọkpọ ikuku ọkụ
Brick mejupụtara obere ihe na -akpụ akpụ maka ọkpọ ikuku ọkụ
Ụdị ihe ọ bụla na -emegharị emegharị, atụmatụ ekwenti a haziri ahazi nwere eserese
Uru ngwaahịa: nnukwu ikike nchekwa ọkụ, ọnụego creep dị ala na uru ndị ọzọ.
Ngwa ngwa ngwaahịa: dabara maka ịkwado ọkụ na -enwu ọkụ na ite ọkụ maka obere ọkụ na obere ọkụ.
nkọwa ngwaahịa
A na-eji brik mebere brik mejupụtara obere ikuku maka ọwa ikuku na-ekpo ọkụ dị ka akụrụngwa bụ isi, nke agbakwunyere site na mgbakwunye pụrụ iche, site na nnukwu nrụgide, wee gbaa ya ọkụ na oke okpomọkụ. Ọ nwere uru nke nnukwu nchekwa nchekwa ọkụ yana ọnụego creep dị ala.
Ngosipụta anụ ahụ na kemịkal
oru ngo | DRL-135 | DRL-145 | DRL-150 | DRL-165 | DRL-155 | DRL-48 |
Al2O3,% ≥ | 70 | 75 | 80 | 65 | 55 | 48 |
Refractoriness ≥ ≥ | 1790 | 1790 | 1790 | 1790 | 1770 | 1750 |
Porosity pụtara% ≤ | 20 | 20 | 19 | 24 | 24 | 24 |
Ike mkpakọ na ụlọ okpomọkụ MPa ≥ | 65 | 70 | 80 | 49 | 44.1 | 39.2 |
Mgbanwe ọnụego nke reheating waya% ≥ | ± 0.1 | ± 0.1 | ± 0.1 | + 0.1 ~ -0.4 | + 0.1 ~ -0.4 | + 0.1 ~ -0.4 |
1450 ℃*2h | 1500 ℃*x2h | 1450 ℃*2h | ||||
Ibu ọkụ na -eme ka ọ dị nro (0.2Mpa) ≥ ≥ | 1500 | 1550 | 1650 | 1500 | 1470 | 1420 |
Ọnụ mbelata% ≤ | 0.6 1350 × h 50h |
0.6 | 0.7 | – | – | – |
1450 × h 50h | 1500 × h 50h | – | – | – |