Okwu mmalite nke epoxy pipe n’ichepụta usoro

Okwu Mmalite nke epoxy ọkpọkọ n’ichepụta usoro

1. Nkwadebe nke gluu. Kpoo resin epoxy n’ime mmiri ịsa ahụ ruo 85 ~ 90 ℃, gbakwunye onye na-agwọ ọrịa dịka onye na-agwọ ọrịa resin / na-agwọ ọrịa (mass ratio) = 100/45, kpalie na igbari ya, na-echekwa ya na gluu tank n’okpuru ọnọdụ nke 80-85 ℃. .

2. The iko eriri na-emerụ na metal gburugburu isi ebu, longitudinal winding n’akuku bụ banyere 45 °, na obosara nke eriri yarn bụ 2.5mm. Igwe eriri eriri bụ: winding ogologo 3.5mm gbara ọkpụrụkpụ + hoop winding 2 layers + longitudinal winding 3.5mm thick + 2 windings.

3. Hichaa mmiri mmiri resin gluu iji mee ka ọdịnaya gluu dị na oyi akwa ikuku na-agbakọ dị ka 26%.

4. Tinye tube plastic na-ekpo ọkụ na-ekpo ọkụ na oyi akwa nke dị n’elu, fesa ikuku na-ekpo ọkụ ka ọ daa ma kechie ya nke ọma, wee kechie oyi akwa nke dị n’èzí na akwa 0.2mm, teepu akwa iko 20mm n’akụkụ mgbanaka, wee ziga ya na ya. oven na-ekpo ọkụ maka ịgwọ ọrịa.

  1. Ngwọta nchịkwa, nke mbụ na-ebili site na ọnụ ụlọ okpomọkụ ruo 95 ° C na ọnụego 3 ° C / 10min, debe ya maka 3h, wee bulie ya na 160 ° C n’otu okpomọkụ ahụ, debe ya maka 4h, wee wepụ ya na XNUMXh. oven ma mee ka ọ dị jụụ ruo n’ime ụlọ.

6. Demould, wepụ ihe iko ákwà teepu n’elu, na-eme post-processing dị ka mkpa.